The organization to ensure that specified requirements are met and agreed upon during all phases of gray iron castings, ductile and bound, has developed a set of documents that define and describe the operational arrangements of the phases / sub-phases of construction Mergers and follows very closely the services that run with external partners as heat treatment and painting.

 

HARDNESS CLASSIFICATION

European law: : EN 1561:1998

DESIGNATION Thickness of determining wall Brinell hardness HB30
greater than less than or
equal to
min. max.
EN-GJL-HB 155 40 80 - 155
20 40 - 160
10 20 - 170
5 10 - 185
2,5 5 - 210
EN-GJL-HB 175 40 80 100 175
20 40 110 185
10 20 125 205
5 10 140 225
2,5 5 170 260
EN-GJL-HB 195 40 80 120 195
20 40 135 210
10 20 150 230
5 10 170 260
4 5 190 275
EN-GJL-HB 215 40 80 145 215
20 40 160 235
10 20 180 255
5 10 200 275
EN-GJL-HB 235 40 80 165 235
20 40 180 255
10 20 200 275
EN-GJL-HB 255 40 80 185 255
20 40 200 275

 

CLASSIFICATION ACCORDING TO TENSILE STRENGTH

European law : EN 1561:1998

DESIGNATION Tensile strength
Rm min.
MPa
EN-GJL-100 da 100 a 200
EN-GJL-150 da 150 a 250
EN-GJL-200 da 200 a 300
EN-GJL-250 da 250 a 350
EN-GJL-300 da 300 a 400
EN-GJL-350 da 350 a 450